3 GOLDEN RULES FOR CLINKER COOLER

Previous Post
Next Post

3 GOLDEN RULES FOR CLINKER COOLER

 

Attention!! to Download Most Important Books in Cement industry reviewed from more than two thousands people + Manuals and noted from big Cement Companies like F L  S , Holcim Lafarge , Cemex , + Excel sheets for calculations process Click here Now 

 

 

TARGETS  of the Clinker Cooler

1) Heat recuperation from hot clinker
to minimize the required fuel input   (combustion) for   the kiln system

2) Cooling of clinker

Target 100 – 150 °C clinker outlet temperature
for easy clinker conveying, clinker storage and   cement grinding

 

Grate Cooler Process Terminology

 

Grate Cooler Equipment Terminology

 

Grate Assembly

 

Principle of Grate Movement

 

The Clinker Cooler House

 

Typical Weaknesses of Older Coolers

  • No static cooler inlet section
  • Outdated grate plate technology (e.g. Folax or Volga plates)
  • Misalignment of grate
  • Internal drag chain
  • Beam aeration
  • Large compartments
  • High grate area load [t/d/m2]
  • Low grate width load [t/d/m]
  • Low specific cooling air [Nm3/kgcli]
  • Grate geometry (steps, inclination)
  • No reliable process indicators
  • Manual control without interlocks
  • Mechanical grate drive
  • Hammer crusher

1st rule: Keep the clinker on the grates = minimize clinker fall through>improve gap management

 

Cooler grate plates are designed to carry the hot clinker bed and are made of heat-resistant steel.

The rest of the cooler is not designed for such high temperatures; particularly the supporting structure beneath the grate must not be exposed to more than 200°C.

Hot clinker must be prevented from spilling through the grate by keeping all functional gaps tight (gap management).

 

2nd rule:

Controlled air distribution into the clinker
>minimize air losses
> compartment sealing required !!!

Cooling air must follow the intended channels and cool the intended areas.

This cannot be achieved if the cooler leaks air through worn plates, gaps, poor compartment seals, or leaking hopper discharge valves.

Also, intake of false air through the kiln outlet seal, clinker crusher, or cooler exhaust-air system must be minimized.

Unsealed compartments

3rd rule:

Operate with high clinker bed
> low grate speed
> increased heat recuperation

 

A high clinker bed increases the residence time of the air in the clinker, essential for good heat exchange.

The cooler should always be operated at the lowest possible grate speed.

Cooling Time – Retention Time

Keeping the Clinker on the Grate is the Key

 

Gap Management

Overview Grate Plates: Air openings

Grate Plates: Gap between the plates

Template to check Dimensions on Grate Plates

Red river formation / excessive wear on side

 

Overview Side Plate Design

 

Hardfacing to Maintain the Side Gap

 

Misaligned Grate Movement

Wear on Support Rollers and Wedges

 

Wear on the Wedges

Targets for gaps on the grate arrangement

1.Gap between the grate plates: max. 2 mm

2.Gap between fixed and movable row: 1 mm

3.Gap between movable and fixed row: 3 mm

4.Side gap:

-5 to 7 mm if side plates are fixed on side walls

-2 mm on movable rows if side plates are fixed on the fixed grate plate supports (0 mm in the area of the fixed grate plates supports)

5.Grate guidance: 0.25 mm on each side of the guide roller
(Max 1 mm in total)

Measure:

If required minimize gaps with spacers or  weld-on front pieces

Rules for the grate re-alignment

 

1.Replace deformed and worn out equipment.

-Steel frames deformed > 5 mm

-Support rollers and wedges worn out > 3 mm

-Grate plates with a remaining thickness < 8 mm

-Washed out side plates

2.Establish quality standards and quality control for key parts (grate plates, grate plate supports, side plates, support rollers and wedges)

3.Use centre position (centre of stroke length) of the grate as reference for the grate alignment

4.Minimize shimming.
If shimming is required fix the shims by welding

5.Avoid shearing forces for screw connections

6.Assure plate fixation by tack welding

7.If required minimize gaps with spacers or weld-on front pieces

Final Messages Gap Management

> Detect and eliminate design weaknesses

>  Establish quality standards for grate equipment

>  Preventive maintenance is essential

>  A general grate alignment is required every 3 to 5 years minimum

Target:  No unexpected stops due to cooler failures

Static Cooler Inlet Section: Requirements

  • Rapid clinker cooling to avoid clinker agglomeration
    (clinker liquid phase)
  • Clinker distribution from the drop point to the entire grate width (horse shoe)
  • Reduced thermal load of the grate equipment (operational safety)
  • 100% sealed (no air losses)

Criteria for Static inlet

  • Adequate number of air cannons required.(vessel size min. 100 liter; nozzles required)
  • Installed specific aeration min. 1.8 m3/m2/s.
  • Static pressure of the fans min. of 100 mbar under grate pressure.
  • Downwards slopped grate plate (5° to 8°) to create downhill force for big lumps
  • Static (dead) clinker layer on the grate plates before start-up
  • Burn tip position: 500 to 1000 inside cold kiln
  • Clinker drop height: > 4 meter
  • Sufficient air required already during start-up

Layout Details

Horse Shoe Layout (Concept A with inclined walls)

Horse Shoe Design and Air Blaster Location

Measures to Minimize Snow Man Formation

1.Design of static cooler inlet (horse shoe)

2.Air Blaster location

3.Air blaster operation (sequence)

4.Specific aeration of the cooler inlet

5.Manual measures to get rid of snow man

Specific Aeration of the Static Cooler Inlet

Manual Measures to Destroy a Snowman

High/low operation:

1.Pile up clinker behind the snow man by decreasing grate speed and flow on the static inlet

2.Shoot the air cannons manually

3.Increase grate speed and flow that the snow man can flow down the static inlet

4.Repeat this procedure (high/low operation) after 15 minutes if required

5.In hard cases the use of poles, lances or cardox might be required

Sufficient air required already during start-up

Air Distribution: Clinker Temperature Profiles

Hot clinker at the cooler inlet and at the border sides
= high pressure resistance.

Cold clinker at the cooler outlet and in the centre of the grate
= low pressure resistance.

The cooling air escapes in aeras of low pressure resistance.

> Small aeration field in the recuperation zone and a good chamber sealing is required !!!

Target:Minimize cooling air losses to cold clinker areas

Air Distribution Template

Aeration Scheme / Air distribution

Clinker Cooling Curve and Air Distribution

Clinker Cooling Curve Calculation

 

Cooling air fans

  • Undergrate pressure
  • Fan curve
  • Fan calibration
  • Fan assessment

Pressure Drop of the Aeration System

Clinker Pressure Drop = f (Clinker Temperature)

Fan Curve, Pressure Resistance Curve

Recommended Fan Speed

Fan Calibration

Situation: CCR flow indications are not reliable

Recommended measures:

Fan calibration by automation and process team

Fans: Air Flow Calibration

Fan Assessment:Example

Compartment Sealing

What is the Partition Wall?

A barrier between the different chambers, to avoid air escape from a chamber with higher pressure to the next chamber with lower pressure

Leakage in Partition Wall

Air Losses via Partition Walls

  • Without barriers the air escapes to the cooler end (less pressure resistance of colder clinker)

Correct Air Distribution

  • The air pressure is adjusted to achieve the following air distribution
  • The partition walls are tight

Installation of hopper sensors

Targets

  • Improve hopper sealing by remaining clinker layer inside the hopper (minimize air losses)

False Air Minimization

> At cooler exhaust air system

>  Kiln nose ring cooling

> Kiln inlet and out seal

> Doors, inspection windows

Target: Reduce cold air intake

Final Messages Controlled Air Distribution

> Improve air distribution and clinker cooling curve

> Fan performance and control is important

>  Compartment sealing is essential

Target: Minimize cooling air losses

Clinker Bed Height

Increased clinker bed height
> increased retention time of air and clinker
> increased cooling time
> improved heat transfer
> improved clinker cooling

Strokes per Minute

Clinker Bed Height

Low clinker bed (< 500 mm)

>Limited air retention time in clinker

>Short clinker retention time in cooler

>Short cooling time

>Low heat transfer

>Risk of grate plate overheating

>High clinker exit temperature

>Low secondary air temperature

>Limited heat recuperation

>Poor cooler efficiency

>Frequent equipment overheating

High clinker bed (> 600 mm)

>Higher air retention time in  clinker

>Long clinker retention time in cooler

>Increased cooling time

>Improved heat transfer

>Best protection for grate plates

>Lower clinker exit temperature

>Higher secondary air temperature

>Increased heat recuperation

>Good cooler efficiency

>Increased cooler availability

Grate Cooler Control Loops

Why Cooling Air (Fan) Control?

>Without control the cooling air flow varies due to pressure drop changes in the clinker bed

>Avoid air losses

> Improve air distribution

Basic Principle of Cooling Air Flow (Fan) Control

Setpoint target: see fan operation table

Actual air flow > setpoint
> fan damper closes or fan speed reduces

Actual air flow < setpoint
>fan damper opens or fan speed increases

Air Flow Table

Why Grate Speed Control?

>Minimize fluctuations of recuperation temperature

>Avoid overfilling of the grate
(downtime for manual emptying of the grate)

> Avoid emptying of the grate
(overheating of the grate plates)

>Grate speed control prevents the clinker bed
resistance from exceeding the pressure capabilities of the cooling air fans

Grate Speed Control (UG Pressure Control)

Basic control principle:

Actual UG pressure > setpoint
> grate speed increase

Actual UG pressure < setpoint
>grate speed decrease

Precondition:

Constant flow of the reference fan

Setpoint of Grate Speed Control

Setpoint = f (reference air flow)

Disturbance of Grate Speed Control

If reference flow is not constant:

> e.g. 3% flow fluctuation
> up to 9% pressure dead band

Grate speed may tend to over and under driving

Grate Speed Control (Level Control)

LevelRadar for direct measuring of the clinker bed height

Guideline for grate speed

Operation Interlocks

MalfunctionAction
Grate drive trippedKiln release taken off after 5 minutes
Fan tripped in cooler inletGrate drive stops after 5 minutes
Fan tripped in remaining recuperation zoneGrate drive stops after 5 to 10 minutes
Fan tripped in cooling zoneGrate drive stops after 15 to 20 minutes
Clinker crusher trippedGrate drive stops immediately
(after 5 minutes)
Clinker transport trippedGrate drive stops immediately
(after 5 minutes)
Cooler exhaust air fan or kiln ID fan trippedGrate drive stops immediately
Cooling air flow reduced to 50%
Cooler exhaust air fan and kiln ID fan trippedGrate drive stops immediately
All cooling air fans off immediately

Main Issues Grate Cooler Control

1.Grate drives and grate speed control have a key function for heat recuperation and clinker cooling

2.Reliable process indication
>Reliable process control + interlocks
> Increased equipment availability

3.If it is not measured it will not be improved

Summary Clinker Cooler

1.Golden rules for clinker cooler are key

2.Gap management

3.Air distribution + fan performance„Air Flow Table“

4.Compartment sealing is essential

5.Clinker bed height = cooling time„Grate Speed Guidelines“

6.Automatic cooler control + interlocks

 

 

 

 

Previous Post
Next Post

Leave a Comment

Your email address will not be published. Required fields are marked *

10 Essential Cement Plant Calculations

Free PDF — clinker chemistry, kiln sizing, ball mill power, and more. Enter your email and we'll send it immediately.

No spam. Unsubscribe anytime.

Check Your Inbox

Your PDF is on its way. Plus 6 more emails with cement plant tips and case studies.