Brown clinker
Brown cement
Brown concrete

 

when you buy the package from here , you will get books + complete Courses + Manuals and Notes from very Reputable companies + confidential Guides and Drawings for Cement industry owned by experts only click here Now.

 

The problem:
Brown concrete

The reason: Brown clinker

Situation

– Sötenich plant:

-Brown cored clinker caused brown cement
and brownish concrete surfaces

-Market focus: pre-cast cement

-Colour of cement / concrete important
-Cement less competitive

-Problems with brown cored clinker is not new
(since years, but increased in 2002)

-but does not always appear

-Sometimes problems with brown stainings
(Fe2+)
-Fuels:

-Lignite, presently animal meal
-Old burner, old grate cooler

Distinguish between:
Colour of cement
Brown stainings due to Fe2+

Study: Find levers to get “black cores”
and grey cement

 

– Several industrial tests: Not successful

-Higher amount of animal meal causes higher amount of Fe2+
-Brown clinker cores even without animal meal
– September 2002: Start of systematic clinker sampling
-Fuels, kiln conditions, clinker chemistry, granulometry
– Study in CTEC-Lab
– Literature study, microscopy, process data, lab burned
clinker granules
– 2003: Investment in new burner

Summary of findings

-What causes dark / light clinker ?
-C4AF is the only dark component in clinker
– Incorporation of Mg leads to dark C4AF – changes lattice
parameters – semi conductive properties leads to dark
colour
-This electrical properties can be disturbed by even small
amounts of other ions. e.g. Fe2+ Mn2+ , Ti4+ or Si4+
– Incorporation only when C4AF crystallizes: > 1250 °C
– Colour depending on condition in sinter zone and
pre-cooling condition (crystallisation) in kiln

What bleaches C4AF in brown cores?

-Fe2+ seems to be the main reason in Sötenich but:
-Fe2+, Mn2+, Ti, Si in clinker cores: no significant differences
detectable, but:
– No Fe2+ in clinker after cooler does not necessarily mean
that no Fe2+ in liquid phase in sinter zone
-Fe2+normally re-oxidised after sinter zone
-but needs time and oxygen
-Fe2+ appears not only due to reducing conditions:
a) reducing atmosphere or flame touching the lining
b) fuel in clinker (too coarse material – solid fuels..)
c) thermal dissociation of Fe3+ in hot sintering zone

-Experience of plants:
-The core is brown and never the surface
– Bigger clinker granules have more often brown cores
– More often when kiln is operated at full capacity
-Hypothesis, resulting from literature study:
-Brown clinker cores seems to be caused by an diffusion effect:
Balance of crystallisation speed of C4AF and re-oxidation of
Fe2+
-Cooling speed > 1250 °C (pre-cooling in kiln)
-O2 content in atmosphere / flame
-Porosity of clinker
-Liquid phase content
– Even when only very few FeO is detectable < 0,04 %) – meaning that
the not incorporated FeO oxidised afterwards

Confirmation of hypothesis
Plant and lab tests

– Analysis of plant clinker samples and process data
-Fuel mix / fuel rates
-burner positions
-Extensive microscopic investigation in CTEC-Lab
-Lab burned clinker with Sötenich raw material
-Different cooling conditions over and below 1250 °C
-Comparison with other raw meals
-Impact of atmosphere
-Impact of Manganese (Sötenich: 0,2 % MnO in clinker)

Analysis of plant clinker samples

 

 

Microscopic examination

– Fast cooling
– Partly reducing conditions
– No difference between brown and black cores
– High amounts of Alkali Aluminate –> Fast stiffening

 

Lab tests to check cooling conditions

– Check of different cooling rates > 1250 °C in lab furnace

Comparison of different conditions

Results of process data an lab test study:

-Brown cores appear, even only very little FeO is
detectable, nevertheless FeO is the cause
-Microscopy investigation – confirms lab burning tests

-Partly reducing conditions due to coarse fuel (lignite +
animal meal) + divergent flame + sometimes thermal
overheating
-Too rapid cooling: No pre-cooling zone in kiln caused by
burner position

– Rather coarse raw mix causes “overheating”
-High Manganese content might boost the effect
-Coarse clinker granules favour brown cores – due to
oxygen diffusion barrier into the core

Recommendations

-Shorter flame – shorter sinter zone
-With old burner not possible
-Convergent flame – not touching the clinker
– With old burner not possible
– Move burner into the kiln in order to lengthen cooling zone
-Detrimental to clinker reactivity
– Finer fuels
– No coal mill in Sötenich

– Finer raw mix decrease coarse Quartz content (raw mill
improvement)

-Increase SO3 in clinker in order to improve burnability and
produce smaller clinker granules (+ increase workability)

Other plant actions

-Manual estimation of clinker colour –>separation
-Only black clinker for precast cement
-Target: Implement automatic colour measurement of press
tablets in auto-lab – result triggers separation of clinker
– Implement FeO quick test
-Separate clinker
– Change fuel mix (reduce
animal meal)
– Result: No claims in 2003

 

 

Previous Post
Next Post

Leave a Comment

Your email address will not be published. Required fields are marked *

10 Essential Cement Plant Calculations

Free PDF — clinker chemistry, kiln sizing, ball mill power, and more. Enter your email and we'll send it immediately.

No spam. Unsubscribe anytime.

Check Your Inbox

Your PDF is on its way. Plus 6 more emails with cement plant tips and case studies.