Kiln Shutdown Procedures

Previous Post
Next Post

Kiln Shutdown Procedures

 

when you buy the package from here , you will get books + complete Courses + Manuals and Notes from very Reputable companies + confidential Guides and Drawings for Cement industry owned by experts only click here Now.

Normal shut-down of the kiln plant

1. Reducing of the kiln feed in steps of 5%, minimal kiln feed is about 40…50%
an empty kiln can be easier heated-up and re-started!
2. Stop of PC-Burner and kiln feed
3. Tertiary air flap to be closed
4. Stop of the main burner (or minimum for a short stop), primary fans to be kept in
operation (cooling!!!)
5. Fresh air flaps to be opened
6. Pre-heater-damper: 10-15% (0% = closed)
7. Stop Pre-heater-fan and adjust the main Bag house-fan damper so that the
pressure after the Pre heater-fan is -1.5 mbar
8 .Cooler fans: minimum speed or dampers to be closed
9.Cooler exhaust air fan: set to minimum to maintain kiln hood draught..
10.Start the kiln on the barring drive. (Aux)
11. Kiln to be tilted! – During cooling down
If raining: run kiln continuously with auxiliary drive
– 1st and 2nd hour each 10 min 120°
– 3rd hour each 15 min 120°
– 4th hour each 20 min 120°
– 5th till 8th hour
– then…each 30 min 120°

…till a kiln shell temperature (sintering zone) of about 100°C is reached
12. Cooler track units: to be operated in intervals

Previous Post
Next Post

Leave a Comment

Your email address will not be published. Required fields are marked *

10 Essential Cement Plant Calculations

Free PDF — clinker chemistry, kiln sizing, ball mill power, and more. Enter your email and we'll send it immediately.

No spam. Unsubscribe anytime.

Check Your Inbox

Your PDF is on its way. Plus 6 more emails with cement plant tips and case studies.

Ask a Cement Engineer ×
Hello! Ask me any cement plant technical question — kiln, grinding, quality, maintenance, preheater. I'll give you a practical answer.