| Loesche – Heat Balance Calculation | |||||||||||||
| Fill in white cells | |||||||||||||
| Composition % | Moisture % | ||||||||||||
| Limestone | 40 | 4 | 5.63 | ||||||||||
| Marl | 50 | 6 | 11.06 | ||||||||||
| Sand | 7 | 10 | 2.67 | ||||||||||
| Iron ore | 3 | 7 | 0.78 | ||||||||||
| Total | 100 | 20.14 | t/h | ||||||||||
| Mill output | 379.86 | t/h | |||||||||||
| Feed | 400 | t/h | |||||||||||
| Moisture on finish product | 0.5 | % | |||||||||||
| Gas Flow Balance | |||||||||||||
| Inputs | Outputs | ||||||||||||
| Amount (t/h) | Nm3/h | % | Nm3/h | % | |||||||||
| Mill inlet gas flow | 330000 | 84.1 | Mill outlet gas flow | 392572 | 100 | ||||||||
| Water from feed | 20.14 | 25176 | 6.4 | ||||||||||
| Water injection | 5 | 6250 | 1.6 | ||||||||||
| False air | 31147 | 7.9 | |||||||||||
| TOTAL | 392572 | 100 | 392572 | 100 | |||||||||
| In a vertical roller mill the % of false air is usely between 5 and 10% | |||||||||||||
| 330000 | Nm3/h on wet | 392572 | Nm3/h on wet | ||||||||||
| Gas coming from the kiln | 270°C | 307230 | Nm3/h on dry | Gas temperature | 100°C | 346248.854 | Nm3/h on dry | ||||||
| % | th/h | % | th/h | ||||||||||
| CO2 | 26.1 | 9687 | CO2 | 23.07 | 3363 | ||||||||
| O2 | 6.77 | 1812 | O2 | 8.39 | 909 | ||||||||
| CO | 0.1 | 26 | CO | 0.06 | 6 | ||||||||
| N2 | 67.2 | 17363 | N2 | 68.53 | 7261 | ||||||||
| H20 | 6.9 | 2250 | H20 | 11.8 | 1654 | ||||||||
| 100.17 | 31137 | 100.05 | 13193 | 17944 | 17496 | -2.496 | |||||||
| Heat balance | |||||||||||||
| Inputs | Outputs | ||||||||||||
| t/h or Nm3/h | T° (°C) | kCal/Nm3 | th/h | th/toutput | % | t/h or Nm3/h | T° (°C) | kCal/Nm3 | th/h | th/toutput | % | ||
| or kCal/kg | or kCal/kg | ||||||||||||
| Hot gases from kiln | 330000 | 270 | 31137 | 81.97 | 85.2 | Gases | 392572 | 100 | 13193 | 34.7 | 35.4 | ||
| Mill feed | 379.86 | 20 | 3.9 | 1481 | 3.9 | 4.1 | Kiln dust | 21 | 90 | 16.7 | 351 | 0.9 | 0.9 |
| Water from feed | 25176 | 20 | 7 | 176 | 0.5 | 0.5 | |||||||
| Water injection | 6250 | 10 | 3.5 | 22 | 0.1 | 0.1 | Kiln feed | 380 | 90 | 18.5 | 7027 | 18.5 | 18.9 |
| False air | 31147 | 25 | 7.7 | 240 | 0.63 | 0.7 | Water vaporisation | 25.14 | 636 | 15989 | 42.1 | 42.9 | |
| Kiln dust | 21 | 270 | 55 | 1155 | 3.0 | 3.2 | Convexion + radiation | 702 | 1.8 | 1.9 | |||
| Table motor energy | 2353 | 6.2 | 6.4 | ||||||||||
| TOTAL | 36565 | 96.3 | 100.0 | TOTAL | 37263 | 98.1 | 100.0 | ||||||
| Difference | 2 | % |
| ||||||||||
Download from here
To Download this Amazing Excel sheet + all other useful books and manuals and excel sheets Kindly Click HERE NOW

Can’t download the excel sheet
please share excel sheet of loesche heat balance.
pls share excel file